Paslanmaz Çelik Boru Standartları

Paslanmaz çelik boru

news-1-1

Boyutlar: 1/8″ ila 24″
Sınıf: 304H, 316H, 309/S, 310/S, 317/L, 321/H, 347/H, 904L, 330, 254SMO, 410.
Özellikler: ASTM A312, ASTM A358, ASTM A813, ASTM A814

Paslanmaz çelik borunun kalitesi

Malzeme ASTM Sınıfı UNS Sınıfı DIN Sınıfı JIS Notu Çelik Adı
östenitik TP 304 Serisi S30400 1.4301 SUS304TB X5CrNi18-20
TP 304L S30403 1.4306   X2CrNi19-11
TP 304L S30403 1.4307 SUS304LTB X2CrNi18-9
TP 304H S30409 1.4948 SUS304HTB X6CrNi18-10
TP 310S S31008 1.4845 SUS310STB X8CrNi25-21
TP 310H S31009      
    1.4335   X1CrNi25-21
TP 316 S31600 1.4401 SUS316TB X5CrNiMo17-12-2
TP 316L S31603 1.4404 SUS316LTB X2CrNiMo17-12-2
TP 316H S31609 1.4918 SUS316HTB X6CrNiMo17-13-2
TP 316Ti S31635 1.4571 SUS316TiTB X6CrNiMo17-12-2
TP 321 S32100 1.4541 SUS321TB X6CrNiNb18-10
TP 312H S32109 1.4941 SUS321HTB X6CrNiTiB18-10
TP 347 S34700 1.455 SUS347TB X6CrNiNb18-10
TP 347H S34709 1.4912 SUS347HTB X7CrNiNb18-10
Ferritik ve Martensitik TP 405 S41500 1.4002 SUS 405 TB X6CrAl13
TP 410 S41000 1.4006 SUS 410 TB X12Cr13 Serisi
TP 430 S43000 1.4016 SUS 430 TB X6Cr17 Serisi
Ferritik / Östenitik   UNS S31803      
2205 UNS S32205 1.4462   X2CrNiMoN22-5-3
2507 UNS S32750 1.441   X2CrNiMoN25-7-4
  UNS S32760 1.4501   X2CrNiMoCuWN25-7-4

 

Paslanmaz çelik boru standardı

A 213 / SA 213 Dikişsiz Ferritik ve Östenitik Alaşımlı Çelik Kazan, Kızdırıcı ve Isı Eşanjör Boruları
A 249 / SA 249 Kaynaklı Östenitik Çelik Kazan, Kızdırıcı, Eşanjör ve Kondenser Boruları
A 268 / SA 268 Genel Hizmete Yönelik Dikişsiz ve Kaynaklı Ferritik ve Martensitik Paslanmaz Çelik Borular
A 269 Genel Hizmet için Dikişsiz ve Kaynaklı Östenitik Paslanmaz Çelik Borular
A 312 / SA 312 Dikişsiz, Kaynaklı ve Ağır Soğuk İşlenmiş Östenitik Paslanmaz Çelik Borular
A 376 / SA 376 Yüksek Sıcaklık Hizmeti için Dikişsiz Östenitik Çelik Boru
A 688 / SA 688 Dikişsiz ve Kaynaklı Östenitik Paslanmaz Çelik Besleme Suyu Isıtıcı Boruları
A 789 / SA 789 Genel Hizmet için Dikişsiz ve Kaynaklı Ferritik/Östenitik Paslanmaz Çelik Borular
A 790 / SA 790 Dikişsiz ve Kaynaklı Ferritik/Östenitik Paslanmaz Çelik Boru
A 999 / SA 999 Alaşımlı ve Paslanmaz Çelik Borular için Genel Gereksinim
A 1016 / SA 1016 Ferritik Alaşımlı Çelik, Östenitik Alaşımlı Çelik ve Paslanmaz Çelik Borular için Genel Gereklilik
Avrupa Standardı  
DIN EN 10216-5 Basınç Amaçlı Dikişsiz Çelik Borular
DIN EN 10217-7 Basınç Amaçlı Kaynaklı Çelik Borular
DIN EN 10297-2 Mekanik ve Genel Mühendislik Amaçlı Dikişsiz Çelik Borular
DIN EN 10305-1 Hassas Uygulamaya Yönelik Çelik Borular
Alman Standardı  
DIN 11850 Gıda ve Kimya Endüstrisine Yönelik Paslanmaz Çelik Borular-Boyutlar, Malzemeler
DIN 17455 Genel Amaçlı Kaynaklı Dairesel Paslanmaz Çelik Borular
DIN 17456 Genel Amaçlı Dikişsiz Dairesel Paslanmaz Çelik Borular
DIN 17457 Özel Gereksinime Tabi Kaynaklı Dairesel Östenitik Paslanmaz Çelik Borular
DIN 17458 Özel Gereksinime Tabi Dikişsiz Dairesel Östenitik Paslanmaz Çelik Borular
DIN 28180 Eşanjör için Dikişsiz Çelik Borular
DIN 11850 Gıda, İçecek, Kimya ve İlaç Endüstrisi için Kaynaklı Borular ve Borular
Rus standartı  
GOST 9941 Korozyona Dirençli Çelikten Yapılmış Dikişsiz ve Sıcak Şekillendirilmiş Borular
Norsok Standardı  
Norsok M - 650 Özel Malzeme Üreticilerinin Yeterliliği
Norsok M - 630 Borular için Malzeme Veri Sayfaları ve Eleman Veri Sayfaları

 

Kimyasal Gereksinimler (%)

Seviye UNS Tasarımı C Mn P S Si CR Ni MB Ti Not Teşekkür ederim N Vn Cu CE B Al Diğer
TP304 Serisi S30400 0.08 2 0.045 0.03 1 18.0–20 8.0–11 . . . . . . . . . . . . . . . . . . . . . . . .      
TP304L S30403 0.035 2 0.045 0.03 1 18.0–20 8.0–13 . . . . . . . . . . . . . . . . . . . . . . . .      
TP304H S30409 0.04 – 0.1 2 0.045 0.03 1 18.0–20 8.0–11 . . . . . . . . . . . . . . . . . . . . . . . .      
TP310S Serisi S31008 0.08 2 0.045 0.03 1 24.0- 26 19.0- 22 0.75 . . . . . . . . . . . . . . . . . . . . .      
TP310H (İngilizce) S31009 0.04 - 0.1 2 0.045 0.03 1 24.0–26 19.0–22 . . . . . . . . . . . . . . . . . .   . . .      
TP310H (İngilizce) S31035 0.04 - 0.1 0.6 0.025 0.015 0.4 21.5–23.5 23.5–26.5 . . . . . . 0.40- 0.6 . . . 0.20- 0.3 . . . 2.5- 3.5 . . . 0.002- 0.008   Spesifikasyona bakın
TP316 Serisi S31600 0.08 2 0.045 0.03 1 16.0–18 10.0–14 2.00–3 . . . . . . . . . . . . . . . . . . . . .      
TP316L S31603 0.035 2 0.045 0.03 1 16.0–18 10.0–14 2.00–3 . . . . . . . . . . . . . . . . . . . . .      
TP316H S31609 0.04 – 0.1 2 0.045 0.03 1 16.0–18 10.0–14 2.00–3 . . . . . . . . . . . . . . . . . . . . .      
TP317 Serisi S31700 0.08 2 0.045 0.03 1 18.0–20 11.0–15 3.0–4 . . . . . . . . . . . . . . . . . . . . .      
TP317L S31703 0.035 2 0.045 0.03 1 18.0–20 11.0–15 3.0–4 . . . . . . . . . . . . . . . . . . . . .      
TP321 Serisi S32100 0.08 2 0.045 0.03 1 17.0–19 9.0–12 . . . Ti 5 × (C+N) minimum, 0,70 maksimum . . . . . . 0.1 . . . . . . . . .      
TP321H S32109 0.04 – 0.1 2 0.045 0.03 1 17.0–19 9.0–12 . . . 4(C+N) dk; 0.70 maksimum . . . . . . 0.1 . . . . . . . . .      
TP321H S32654 0.02 2.0-4 0.03 0.005 0.5 24.0–25 21.0–23 7.0-8 . . . . . . . . . 0.45- 0.55 . . . 0.30-0.6 . . .      
TP321H S33228 0.04 - 0.08 1 0.02 0.015 0.3 26.0–28 31.0–33 . . . . . . 0.60- 1 . . . . . . . . . . . . 0.05 - 0.1   0.025  
TP321H S34565 0.03 5.0-7 0.03 0.01 1 23.0–25 16.0–18 4.0-5 . . . 0.1 . . . 0.40- 0.6 . . . . . . . . .      
TP347 Serisi S34700 0.08 2 0.045 0.03 1 17.0–19 9.0–13 . . . . . . Spesifikasyona bakın . . . . . . . . . . . . . . .      
TP347H S34709 0.04 – 0.1 2 0.045 0.03 1 17.0–19 9.0–13 . . . . . . Spesifikasyona bakın . . . . . . . . . . . . . . .      
Alaşım 20 N08020 0.07 2 0.045 0.035 1 19.0–21 32.0–38 2.0–3 . . . Spesifikasyona bakın Spesifikasyona bakın . . . . . . 3.0– 4 . . . . . . . . .  
Alaşım 20 N08367 0.03 2 0.04 0.03 1 20.0–22 23.5–25.5 6.0–7 . . . . . . . . . 0.18–0.25 . . . 0.75 . . . . . . . . .  
Alaşım 20 N08028 0.03 2.5 0.03 0.03 1 26.0–28 30.0–34 3.0–4           0.60–1.4        
Alaşım 20 N08029 0.02 2 0.025 0.015 0.6 26.0–28 30.0–34 4.0–5           0.6– 1.4        

 

Isıl İşlem Tablosu

Seviye BM
Tanım
Sona ermek Isıtma Sıcaklığı
TP304H S30409, S30415 Soğuk 1900 derece F [1040 derece]
TP304H S30409, S30415 Sıcak 1900 derece F [1040 derece]
TP310H S31009   1900 derece F [1040 derece]
TP310H (İngilizce) S31035   2160-2280 derece F [1180-1250 derece ]
TP316H S31609 Soğuk 1900 derece F [1040 derece]
TP316H S31610 Sıcak 1900 derece F [1040 derece]
TP321H S32109, S32615 Soğuk 2000 derece F [1100 derece]
TP321H S32109, S32615 Sıcak 1925 derece F [1050 derece]
TP321H S32654   2100 derece F [1150 derece]
TP321H S33228   2050-2160 derece F [1120-1180 derece ]
TP321H S34565   2050-2140 derece F [1120-1170 derece ]
TP347H S34709 Soğuk 2000 derece F [1100 derece]
TP347H S34709 Sıcak 1925 derece F [1050 derece]
Alaşım 20 N08020   1700-1850 derece F [925-1010 derece ]
Alaşım 20 N08367   2025 derece F [1110 derece]
Alaşım 20 N08028   2000 derece F [1100 derece]
Alaşım 20 N08029   2000 derece F [1100 derece]

 

Çekme Gereksinimleri

Seviye UNS Tanımı Çekme Dayanımı, min ksi [MPa] Akma Dayanımı, min ksi [MPa] Diğer
TP304 Serisi S30400 75 [515] 30 [205]  
TP304L S30403 70 [485] 25 [170]  
TP304H S30409 75 [515] 30 [205]  
TP304H S30415 87 [600] 42 [290]  
TP310S Serisi S31008 75 [515] 30 [205]  
TP310H (İngilizce) S31009 75 [515] 30 [205]  
TP310H (İngilizce) S31035 95 [655] 45 [310]  
TP316 Serisi S31600 75 [515] 30 [205]  
TP316L S31603 70 [485] 25 [170]  
TP316H S31609 75 [515] 30 [205]  
TP316H S31635 75 [515] 30 [205]  
TP317 Serisi S31700 75 [515] 30 [205]  
TP317L S31703 75 [515] 30 [205]  
TP317L S31725 75 [515] 30 [205]  
TP317L S31726 80 [550] 35 [240]  
TP317L S31727 80 [550] 36 [245]  
TP317L S31730 70 [480] 25 [175]  
TP317L S32053 93 [640] 43 [295]  
TP321 Serisi S32100 75 [515] 30 [205] kaynaklı ve dikişsiz
TP321 Serisi S32100 75 [515] 30 [205] t=0.375 inç.
TP321 Serisi S32100 70 [480] 25 [170] t > 0.375 inç
TP321H S32109 75 [515] 30 [205] kaynaklı ve dikişsiz
TP321H S32109 75 [515] 30 [205] t=0.375 inç.
TP321H S32109 70 [480] 25 [170] t > 0.375 inç
TP321H S32615 80 [550] 32 [320]  
TP321H S32654 109 [750] 62 [430]  
TP321H S33228 73 [500] 27 [185]  
TP321H S34565 115 [795] 60 [415]  
TP347 Serisi S34700 75 [515] 30 [205]  
TP347H S34709 75 [515] 30 [205]  
Alaşım 20 N08020 80 [550] 35 [240]  
Alaşım 20 N08028 73 [500] 31 [214]  
Alaşım 20 N08029 73 [500] 31 [214]  
Alaşım 20 N08367 100 [690] 45 [310] t=0.187 inç.
Alaşım 20 N08367 95 [655] 45 [310] t > 0.187 inç.